No. | Forming situation | Reason | Solution |
1 | Roll up or buildup at the bottom or neck of the bottle | Delay minor blowing time too long | Shorten the delay minor blowing time |
The temperature is too low at the place where the buildup | Raise the heating temperature at the corresponding place in the tube blank | ||
2 | Deformation at bottleneck | Blank head overheat | Check cooling water circulating |
The temperature of the 1st segment heating lamp is too high | Reduce the voltage of 1st segment heating lamp | ||
Air circulation is not equal in the heating case | Check the ventilator fan in the heating case. | ||
3 | Bottom of the bottle too thick | Preheat of bottle bottom not finished | Raise the temperature of heating case |
Blowing too late | Blowing in advance | ||
Advance blowing pressure too low | Increase advance blowing pressure | ||
4 | bottle bottom broken | Humidity not enough, permeation not enough | Increase humidity |
Delay stretching time too long | Shorten delay stretching time | ||
The extension ratio is too large | Reduce extension ratio | ||
The bottom of the tube is blank too thin | Improve bottom design of tube blank | ||
5 | Buckling in the bottle bottom | The temperature of the bottom too high (poor cooling in sprue) | Reduce the temperature of the bottle bottom properly |
Advance blowing too late | Advance blowing 0.1~0.2s ahead | ||
Blowing time too short | Longer blowing time 0.1~0.2s for 1 to 3 times | ||
Advance blowing pressure too low | Increase advance blowing pressure | ||
6 | The bottle bottom is not full | The temperature of bottle bottom too low | Increase the temperature of the bottom of the heating area |
Not enough air release hole or not equal at the bottle bottom of the mold | Add air release holes and make them distribute equally. | ||
Design of stretching rod head not corresponding with the shape of the bottom of the tube blank | Replace stretching rod head | ||
Blowing pressure is not enough | Increase blowing pressure | ||
rate of flow not enough at blowing valve | Wash blowing valve by gasoline | ||
Blowing time too short | Increase blowing time | ||
7 | Decentration on bottle bottom | Related to bottle blank temperature, advance blowing, high-pressure blowing, etc. | Reduce the temperature of bottle blank; faster-stretching speed; check the gap between stretching head and bottom mold; delay advance blowing, and reduce advance blowing pressure; delay high pressure blowing; check whether bottle blank decentration |
Stretching too short | Make sure the stretching rod leaves the bottle bottom for 0.1mm | ||
Delay minor blowing time too short | Increase delay minor blowing time | ||
8 | Bottom becomes white | Temperature too high | Reduce temperature |
Bottle blank too cold | Raise the temperature of the bottle blank | ||
The weight of the bottle blank is too light | Add the weight of the tube blank | ||
The stretching rod shifted from the center line of the bottle | Adjusting the position of the stretching rod | ||
Advance blowing too late, advance blowing pressure too low | Increase advance blowing pressure | ||
The stretching rod didn't reach the bottom | Adjusting the position of the magnet ring switch | ||
Temperature too high | Reduce temperature | ||
The thickness of the tube blank is not equal | Improve the quality of tube blank | ||
Injection density is not equal | Improve the heating | ||
Heating not equal | Check whether the rotation of the tube blank has a problem | ||
9 | The bottle bottom is too thin | Blowing too earlier | Delay blowing time |
The temperature of bottom is too high | Reduce the temperature of the bottom | ||
The bottom of the tube blank is too thin | Increase the thickness of the bottom of the tube blank | ||
10 | Bottle stuck on the base mold | The time of mold closing and base mold raising is not synchro | Faster the raising time for base mold |
Plastic blowing time is too short | Longer the plastic blowing time | ||
11 | Buckling at the middle of the bottle | Blowing time is too short | Longer blowing time 0.1~0.2s for 1 to 3 times |
The temperature of the middle of the bottle is too low | Increase the temperature of the middle of the bottle properly | ||
12 | Crack at the middle of the bottle just after blowing | The whole temperature of the tube blank is too low | Increase the temperature of the whole oven tunnel, increase properly the voltage of the infrared lamp from 1st segment to 7th segment |
Delay minor blowing time is too long | Shorten delay minor blowing time | ||
The temperature difference of every part of the bottle blank is too large | Heating equably | ||
13 | Bottle blank stuck on the stretching rod | No minor blowing or high-pressure air source | Adjust minor blowing and high-pressure air source |
Blowing valve not working | Check whether the blowing valve connected power, whether the industry blowing valve opened | ||
14 | Bottle blank stretched longer, but not expanded | No high-pressure air source | Open high-pressure air source |
Blowing time is too short | Longer blowing time | ||
15 | The upper part of the bottle is too thick | The temperature of the upper part is too low | Increase temperature in the upper part |
the position of the air release hole of the mold is far from the upper part | Adjusting the position of the air release hole | ||
The extension ratio is too low | Increase extension ratio | ||
Blowing ratio of upper part of the bottle is too low | Change the shape of the bottle | ||
The speed of the stretching rod is too slow | Adjusting the speed of the stretching rod | ||
16 | Obvious mold closing line | The pressure for mold closing is not enough | Increase the mold closing pressure, adjust the angle of the support rod for mold closing (<5̊) |
Sealing is too earlier | Move backward the position of position switch of mold closing | ||
17 | Mold closing line with different size | Mold closing is too loosing | Lock tightly the mold base |
18 | The whole bottle is turbid and not transparent | The whole temperature of the bottle blank is not enough | Increase the whole temperature |
19 | The transparent of the bottle is not good | The heating temperature is too high | Reduce the temperature |
The heating time is too long | Shorten the heating time | ||
There is moisture in the compressed air | Removing moisture by dryer | ||
The tube blank is not transparent itself | Improve the quality of tube blank, select to use material, and improve the dryness of the material | ||
Tube blank design is not proper | Improve the size design of tube blank | ||
The blowing ratio is too small | Reduce the diameter of the tube blank | ||
20 | pearly luster and whiten on the bottle | The heating temperature is too low | Raise the temperature or slower the rotation speed |
The thickness of tube blank is unequal | Improve the quality of tube blank | ||
The thickness of the tube blank is too thick, heating permeation is not enough | Reduce the thickness of the tube blank, or try to raise the cover of heating equipment, so as to increase the temperature distribution on the surface of tube blank | ||
21 | There are prints on the bottle | The quality of the tube blank is not good | Check the quality of the tube blank |
Mold not clean | Cleaning the mold | ||
22 | Deformation just after leaving the mold | Blowing time too short | Increase the blowing time |
The temperature of the cooling water is too high | Reduce the temperature of cooling water | ||
23 | Thickness distribution unequal in the axial direction | The temperature of the tube blank is unequal | Adjusting heating temperature |
Advance blowing pressure too low or too high | Increase or reduce advance blowing pressure | ||
Advance blowing too late or too earlier | Earlier or later advance blowing | ||
24 | Deformation after a long time | Bottle blowing pressure too low | Increase bottle blowing pressure |
Bottle blowing is too short | Longer the bottle blowing time | ||
25 | Bending when heating bottle blank | Rotation wrongly when heating bottle blank | Make sure whether touch or hit aluminum baffle board, etc. |
Overheat at partial of bottle blank | Adjusting the output of the heater | ||
Pimple on the bottle blank | Check whether the bottle blank is qualified | ||
26 | The volume of the produced bottle not enough | When at last plastic blowing, didn't blow to form the shape | Check whether there is a jam at the outlet |
Air pressure is not enough for plastic blowing | Check the air circuit and supply source for plastic blowing |